POM-C (Acetal Co-Polymer) | |||||
Also Known As
|
|||||
Typical Machine Settings: Subject To Polymer Grade |
|||||
Nozzle |
Front |
Centre |
Rear |
||
Barrel Temperature |
195 - 220oC |
190 - 205oC |
190 - 205oC |
190 - 205oC |
|
Melt Temperature |
195 - 230oC |
Must be measured with a pyrometer by taking an airshot through the injection machine nozzle. |
|||
Hot Runner Temperature |
195 - 230oC |
||||
Mould Temperature |
85 - 105oC |
Run at upper end of range for best surface finish. |
|||
Injection Rate |
Medium To Fast |
||||
Specific Injection Pressure |
700 - 1050 Bar (10,000 - 25,000psi) |
||||
Screw Back Pressure |
2.0 - 3.5 Bar (30 - 50psi) |
||||
Screw Speed |
Slow To Moderate |
||||
Processing Features |
|||||
Structure |
Semi-Crystalline |
||||
Specific Gravity |
1.42 |
||||
Viscosity |
Medium |
Needs average size runners. |
|||
Shear Rate Susceptibility |
Medium |
Needs average size gates. |
|||
Temperature Window |
Narrow |
Needs accurate & stable control |
|||
Residence Time |
Short |
Aim for '1-Shot' residence time |
|||
Start-Up Precedure |
|||||
|
|||||
Shut-Down Precedure |
|||||
|